← All published pairs

Acrylic adhesive on HIPS

8 verified lap-shear rows from manufacturer datasheets. Values stay with the surface preparation printed on the sheet.

ProductPrepStrengthStandardSource
3M Scotch-Weld Structural Plastic Adhesive DP8010NS Blue

Overlap Shear (psi), ASTM D1002. DP8010NS Blue column: Polystyrene (HIPS) 570. Cured 7 days at room temperature.

abraded3.93 MPaASTM D1002TDS p.3
3M Scotch-Weld Acrylic Adhesive DP8410NS

Overlap Shear Strength … Dwell Time: 24 h … Test Method: ASTM D1002, ISO 4587 … 23 °C Polystyrene (HIPS) 3.8 MPa (550 lb/in²) (AF) ¹

abraded3.8 MPaASTM D1002, ISO 4587TDS p.3
3M Scotch-Weld Acrylic Adhesive DP8425NS

Overlap Shear Strength … Dwell Time: 24 h … Test Method: ASTM D1002, ISO 4587 … 23 °C Polystyrene (HIPS) 3.8 MPa (550 lb/in²) (SF) ¹

abraded3.8 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Low Odor Acrylic Adhesive DP8810NS

Overlap Shear Strength … Surface Prep: Light Abrasion and Solvent Clean … Dwell Time: 7 d … Test Method: ASTM D1002, ISO 4587 … Polystyrene (HIPS) 3.8 MPa (550 lb/in²) (AF) ¹

abraded3.8 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Acrylic Adhesive DP8405NS

Overlap Shear Strength, 24 h, ASTM D1002, ISO 4587. Polystyrene (HIPS), light abrasion and solvent clean, 3.4 MPa (500 lb/in²).

abraded3.4 MPaASTM D1002, ISO 4587TDS p.3
3M Scotch-Weld Low Odor Acrylic Adhesive DP8805NS

Overlap Shear Strength … Surface Prep: Light Abrasion and Solvent Clean … Dwell Time: 7 d … Test Method: ASTM D1002, ISO 4587 … Polystyrene (HIPS) 3.4 MPa (500 lb/in²) (AF) ¹

abraded3.4 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Low Odor Acrylic Adhesive DP8825NS

Overlap Shear Strength … Surface Prep: Light Abrasion and Solvent Clean … Dwell Time: 7 d … Test Method: ASTM D1002, ISO 4587 … Polystyrene (HIPS) 3.4 MPa (500 lb/in²) (AF) ¹

abraded3.4 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Metal Bonder Acrylic Adhesive DP8407NS

23 °C Polystyrene (HIPS) 3.1 MPa (450 lb/in²) (SF )

abraded3.1 MPaASTM D1002, ISO 4587TDS p.p3

HIPS material page