← All published pairs

Two-part epoxy on Fiberglass

22 verified lap-shear rows from manufacturer datasheets. Values stay with the surface preparation printed on the sheet.

ProductPrepStrengthStandardSource
3M Scotch-Weld Epoxy Adhesive 6101

Overlap Shear Strength … Test Condition: 1 hr at 65 °C + 24 hr at 23 °C … Test Method: ASTM D1002, ISO 4587 … FR-4 36 MPa (Mixed Mode Failure ) ³

not stated36 MPaASTM D1002, ISO 4587TDS p.3
SikaPower-1280

Tensile lap-shear strength (CQP046-9 / ISO 4587) 25 MPa A, C

not stated25 MPaCQP046-9 / ISO 4587TDS p.p1
3M Scotch-Weld Epoxy Adhesive LSB360NS

Overlap Shear Strength Temperature: 23 °C (73 °F) Dwell Time: 7 d Test Method: ASTM D1002, ISO 4587 Substrate Surface Prep Value … FRP (Epoxy) IPA Wipe/Abrade/IPA Wipe 3000 lb/in² (CF )

abraded20.68 MPaASTM D1002, ISO 4587TDS p.2
SikaPower-830

Tensile lap-shear strength (CQP046-9 / ISO 4587) 20 MPa C, D

not stated20 MPaCQP046-9 / ISO 4587TDS p.p1
3M Scotch-Weld Epoxy Adhesive DP490

Overlap Shear Strength Temperature: 23 °C (73 °F) Dwell Time: 7 d Test Method Test Condition Substrate Surface Prep Value … ASTM D1002, ISO 4587 CRF Epoxy IPA Wipe 19 MPa (2756 lb/in²) (AF/CF )

degreased19 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Epoxy Adhesive LSB60

Overlap Shear Strength Temperature: 23 °C (73 °F) Dwell Time: 7 d Test Method: ASTM D1002, ISO 4587 Substrate Surface Prep Value … FRP (Polyester) IPA Wipe/Abrade/IPA Wipe 2700 lb/in² (SF )

abraded18.62 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Epoxy Adhesive DP270 Black

Overlap Shear Strength Temperature: 23 °C (73 °F) Dwell Time: 7 d Test Method: ASTM D1002, ISO 4587 Test Condition Substrate Surface Prep Value … 23 °C FR-4 Solvent Wipe 15.3 MPa (2220 lb/in²)

degreased15.3 MPaASTM D1002, ISO 4587TDS p.3
3M Scotch-Weld Epoxy Adhesive LSB60NS

Overlap Shear Strength Temperature: 23 °C (73 °F) Dwell Time: 7 d Test Method: ASTM D1002, ISO 4587 Substrate Surface Prep Value … FRP (Polyester) IPA Wipe/Abrade/IPA Wipe 2200 lb/in² (SF )

abraded15.17 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Epoxy Adhesive DP270 Clear

Overlap Shear Strength Temperature: 23 °C (73 °F) Dwell Time: 7 d Test Method: ASTM D1002, ISO 4587 Test Condition Substrate Surface Prep Value … 23 °C FR-4 Solvent Wipe 14.3 MPa (2070 lb/in²)

degreased14.3 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Epoxy Adhesive DP125 Gray

Overlap Shear Strength Temperature: 23 °C (73 °F) Test Method: ASTM D1002, ISO 4587 Dwell Time Substrate Surface Prep Value … 7 d FRP (Polyester) Acetone/Abrade/Acetone 12.6 MPa (1830 lb/in²)

abraded12.6 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Epoxy Adhesive DP125 Translucent

Overlap Shear Strength Temperature: 23 °C (73 °F) Test Method: ASTM D1002, ISO 4587 Dwell Time Substrate Surface Prep Value … 7 d FRP (Polyester) Acetone/Abrade/Acetone 10.3 MPa (1500 lb/in²)

abraded10.3 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Epoxy Adhesive DP420 Off-White

Overlap Shear Strength Temperature: 23 °C (73 °F) Test Method: ASTM D1002, ISO 4587 Dwell Time Substrate Surface Prep Value … 7 d FRP (Polyester) Acetone/Abrade/Acetone 9.9 MPa (1440 lb/in²)

abraded9.9 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Epoxy Adhesive DP460NS

Overlap Shear Strength Temperature: 23 °C (73 °F) Dwell Time: 7 d Test Method: ASTM D1002, ISO 4587 Substrate Surface Prep Value … Fiber-Reinforced Plastic IPA Wipe/Abrade/IPA Wipe 1379 lb/in² (SF )

abraded9.51 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Epoxy Adhesive DP190 Translucent

Overlap Shear Strength Temperature: 23 °C (73 °F) Test Method: ASTM D1002, ISO 4587 Dwell Time Substrate Surface Prep Value … 7 d FRP (Polyester) Acetone/Abrade/Acetone 9.2 MPa (1340 lb/in²)

abraded9.2 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Epoxy Adhesive DP420NS Black

Overlap Shear Strength Temperature: 23 °C (73 °F) Test Method: ASTM D1002, ISO 4587 Dwell Time Substrate Surface Prep Value … 7 d FRP (Polyester) Acetone/Abrade/Acetone 7.9 MPa (1140 lb/in²)

abraded7.9 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Epoxy Adhesive DP420 Black

Overlap Shear Strength Temperature: 23 °C (73 °F) Test Method: ASTM D1002, ISO 4587 Dwell Time Substrate Surface Prep Value … 7 d FRP (Polyester) Acetone/Abrade/Acetone 7.3 MPa (1060 lb/in²)

abraded7.3 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Epoxy Adhesive DP460 Off-White

Overlap Shear Strength Temperature: 23 °C (73 °F) Dwell Time: 7 d Test Method: ASTM D1002, ISO 4587 Substrate Surface Prep Value … Fiber-Reinforced Plastic IPA Wipe/Abrade/IPA Wipe 6.9 MPa (1000 lb/in²) (SF )

abraded6.9 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Epoxy Adhesive DP100 Clear

Overlap Shear Strength … Dwell Time: 7 d … Test Method: ASTM D1002, ISO 4587 … Fiber-Reinforced Plastic IPA Wipe/Abrade/IPA Wipe 6.6 MPa (950 lb/in²) ¹

abraded6.6 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Epoxy Adhesive DP405

Overlap Shear Strength Temperature: 23 °C (73 °F) Test Method: ASTM D1002, ISO 4587 Dwell Time Substrate Surface Prep Value … 7 d FRP (Polyester) Acetone/Abrade/Acetone 6.3 MPa (910 lb/in²)

abraded6.3 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Epoxy Adhesive DP270 Black

Overlap Shear Strength Temperature: 23 °C (73 °F) Dwell Time: 7 d Test Method: ASTM D1002, ISO 4587 Test Condition Substrate Surface Prep Value … FRP (Polyester) IPA Wipe/Abrade/IPA Wipe 6.1 MPa (880 lb/in²)

abraded6.1 MPaASTM D1002, ISO 4587TDS p.2
3M Scotch-Weld Epoxy Adhesive DP270 Clear

Overlap Shear Strength Temperature: 23 °C (73 °F) Dwell Time: 7 d Test Method: ASTM D1002, ISO 4587 Test Condition Substrate Surface Prep Value … FRP (Polyester) IPA Wipe/Abrade/IPA Wipe 6.1 MPa (880 lb/in²)

abraded6.1 MPaASTM D1002, ISO 4587TDS p.3
3M Scotch-Weld Epoxy Adhesive DP100NS

Overlap Shear Strength … Dwell Time: 7 d … Test Method: ASTM D1002, ISO 4587 … Fiber-Reinforced Plastic IPA Wipe/Abrade/IPA Wipe 680 lb/in² ¹

abraded4.69 MPaASTM D1002, ISO 4587TDS p.2

Fiberglass material page